Does Passivation Change Thread or Slit Size?

Table of Contents
What does trivalent chrome passivation actually add?
How thick is the film, and does 0.1 µm move a thread or slit?
Why mask threads and mating faces if the film is that thin?
What changes after passivation — color, salt spray, nothing else?
What should the drawing say about passivation?

Passivation does not change the thread or the slit on this cross clamp block. The trivalent chrome film is under 0.1 µm, or 0.0001 mm, and the 0.10 mm feeler that guards the slit is a thousand times thicker. Whatever pushes a thread off go/no-go, this film isn't it.

The part is a 110±10 g Zamak 5 (ASTM B86 AC41A) zinc die casting, 38×38×24 mm, run 1×4 with melt at 400–420 °C and mold at 170–190 °C. Arms sit at 18.0±0.1 mm, the center boss at Ø20×4 mm, and the M10×1.5 thread runs 16 mm deep. The slit is 1.0±0.1 mm wide and 22 mm deep.

What does trivalent chrome passivation actually add?

What it adds is a conversion coating on the zinc itself. Acid takes a little zinc off, and the chromium comes back as a mixed oxide in the same place. Some of that oxide occupies space the zinc gave up, so the film adds almost nothing above the original surface the way plating does.

Die casting passivation is the last wet step before packing, so it must leave every gauge reading where the saw left it. What it buys is time: freshly cut zinc stains within days in humid air, and the oxide slows that corrosion. Hexavalent chromium drops out, capped by RoHS at 0.1% by weight (Directive 2011/65/EU).

How thick is the film, and does 0.1 µm move a thread or slit?

Trivalent films on zinc run 0.03–0.15 µm (typical), and this drawing caps the film at 0.1 µm. At that thickness neither feature moves. Hexavalent chromate, behind the old thickness callouts, ran 0.3–1 µm (typical).

Do the arithmetic. An M10×1.5 flank stands at 60°, and allowance on that form runs four times the film thickness, so 0.1 µm on the flanks moves the pitch diameter 0.4 µm. A 6H/6g fit at this size holds a band well over 0.1 mm (ISO 965-1), so the film takes up under one part in two hundred of it.

On the slit, two coated faces close the gap by 0.0002 mm, and the feeler keeps 0.0998 mm of room at mid-depth.

Why mask threads and mating faces if the film is that thin?

Masking is process hygiene: the bath is an acid, and the thread is a blind hole that rinsing cannot empty. The 16 mm deep thread holds liquid like a cup, and trivalent chemistry that weeps from the root hours later leaves a stain or a soft flank.

The bottom face carries 0.05 mm flatness and acts as the clamp datum. A passivated face with rack marks turns a flatness argument into a finish argument, and the film changes friction, so the same torque seats a different clamp load between lots.

A go/no-go plug run after passivation also drags over film that is still soft, scuffs it, and the scuff reads as a thread defect.

What changes after passivation — color, salt spray, nothing else?

Two things change: color and corrosion resistance. A clear trivalent film reads silver with a faint blue cast, less yellow than the hexavalent iridescence it replaced. Polished faces keep their gloss, and a dye pushes the film to black instead.

The drawing target is 48 h in ASTM B117, and it stays a target until a production lot runs and its coupons come back. Set 48 h on the drawing and let the first article report confirm it.

The inspection sheet stays put: mass, arms, boss, thread go/no-go, slit, feeler, flatness. Contact resistance does move, because the film is not a conductor.

What should the drawing say about passivation?

One line: trivalent chromium passivation, clear, film ≤0.1 µm, threads and mating faces masked, tested to ASTM B201. A second covers salt spray at 48 h, confirmed on the first article. Add that passivation is a finish, and size comes from the tool and the saw.

Mark the masked zones on the drawing itself. The inspection sheet needs the table below.

ItemTargetCheck
Thread M10×1.5, 16 mm deepFull thread, go/no-goPlug gauge, before and after passivation
Slit, 22 mm deep1.0±0.1 mm1.1 mm pin no-go; feeler blocked at mid-depth
Passivation filmTrivalent chrome, clear, <0.1 µmASTM B201 on a lot coupon
Masked zonesThread and mating face film-freeVisual at 10×; plug gauge runs clean
Salt sprayASTM B117, 48 h targetCoupon per lot; first-article confirmation

Before the saw is set, send the drawing for a manufacturability review with the masked zones and the salt spray line marked.