A die casting saw cut is checked in three places, not one. The 1.0±0.1 mm callout is the kerf at the mouth; the 22 mm callout is depth from the entry face; at mid-depth, a 0.10 mm feeler must not enter.
The part is a 110±10 g Zamak 5 (ASTM B86 AC41A) zinc die casting, 38×38×24 mm, with 18.0±0.1 mm arms and an M10×1.5 thread 16 mm deep. The slit crosses that thread.
The mouth is a bad witness: the blade enters there, so the gap stays open. The root is a bad witness too: 22 mm of cut in a 24 mm block leaves only a 2 mm web, and the web stiffens the root. Mid-depth sits away from both.
A tilted blade shows its offset and the halves are free to close. A 1.0 mm blade cutting 22 mm deep can wander under side load. Measure 11 mm down from the entry face and you catch the bow before the root. Measure only the mouth, and a slit that closes at depth still looks wide.
No single gauge does. A depth gauge reads 22 mm from the entry face to the root; it does not read width. A pin gauge or projector reads width at the mouth; it does not read depth. The 0.10 mm feeler reads closure at mid-depth, a third property.
For depth, use a depth gauge with a probe thin enough for the 1.0 mm slot, zeroed on the entry face. A 22.0 mm reading on the 24 mm block leaves a 2.0 mm web. For width, the pin gauge is go/no-go: a 0.9 mm pin must enter, a 1.1 mm pin must not. A projector does the same on a sample.
Pass means the blade stops at the side opening. Fail means it slides in. Offer a 0.10 mm blade at 11 mm below the entry face, perpendicular to the cut faces. Do not wedge, and do not test at the mouth. A 0.10 mm blade can enter a 1.0 mm mouth; that is geometry, not a defect.
The feeler is a closure gauge. A gap that takes the 0.10 mm blade says the cut stayed open. Closing the slit then takes up that gap before the faces seat, and the halves can shift off line. If the blade enters at mid-depth, reject the part and check the saw setup.
Start with the angle. A 0.2 mm offset over 22 mm is 0.52°; 0.2 mm is the full ±0.1 mm band. Four things produce it.
Blade runout is first: 0.05 mm each way at the edge cuts 1.1 mm on one wall, 0.9 mm on the other; side load pushes it deeper. Fixture datum is second: clamp the four arms without seating the bottom face, and the cut tilts. Stress release is third. Melt at 400–420 °C, mold at 170–190 °C, and injection at 25–35 MPa (typical) leave the Ø20×4 mm boss and 8 mm arms at different stress states; cutting one side lets that stress move the other. Re-clamping after deburr is a fourth.
Check drift by cavity on the 1×4 tool. If all four lean the same way, suspect the blade or fixture; if one leans, suspect its fill and stress.
The slit needs three callouts: 1.0±0.1 mm at the mouth as kerf width, 22 mm deep from the entry face, and 0.10 mm maximum gap at mid-depth marked “feeler must not enter.” Add 0.05 mm bottom flatness, a 16 mm deep M10×1.5 thread, and trivalent chromium passivation below 0.1 µm.
The inspection sheet needs datum, gauge, part state, sampling: 0.9 mm pin goes through, 1.1 mm pin does not enter, depth gauge from the entry face, 0.10 mm feeler at 11 mm on a free part. Record the cavity number; cavity-linked drift is not a saw problem.
| Parameter | Target | Check |
|---|---|---|
| Slit width | 1.0±0.1 mm | 0.9 mm pin enters; 1.1 mm pin no-go; projector |
| Slit depth | 22 mm from entry face | Depth gauge; 2 mm web |
| Mid-depth closure | 0.10 mm max | Feeler must not enter |
| Bottom flatness | 0.05 mm | Surface plate; 0.05 mm blade no-go |
Before the first cut, send the drawing for a manufacturability review with the slit, depth, and closure callouts marked.