A 25-tonne hot-chamber machine clamps about 245 kN. That caps projected area, not part weight. This 38×38 mm cross clamp block, run 1×4, needs 9.8–11 tonnes at 30 MPa. The press has margin; area and shot size set the limit.
The part is a 110±10 g Zamak 5 (ASTM B86 AC41A) zinc die casting, 38×38×24 mm, with 18.0±0.1 mm arms and a Ø20×4 mm center boss. The M10×1.5 thread runs 16 mm deep, and the 1.0±0.1 mm slit runs 22 mm. The bottom face holds 0.05 mm flatness. It runs 1×4 in an H13 tool, melt 400–420 °C, mold 170–190 °C, cycle 25–35 s.
Twenty-five tonnes is clamp force: the load that holds the moving platen against the fixed platen. In metric units that is about 245 kN. The rating assumes a stated hydraulic pressure, so the nameplate figure is a ceiling, not a dial setting. It says nothing about part weight. Projected area is the useful figure: at 30 MPa, 245 kN covers about 8,200 mm² across all cavities and the runner. On a given press, the rated tonnage does not change; the part's area does. Compare the layout with that number.
Clamp force equals projected area times injection pressure: F = A × p. Area is the shadow of the cavity, runner, and overflow on the parting line, not the part's surface. Pressure is the metal pressure at the plunger, 25–35 MPa on this zinc part (typical). The units do the work: mm² × MPa gives newtons. For the 1×4 layout, 3,200 mm² at 30 MPa gives 96,000 N, or 96 kN. At 3,600 mm² it gives 108,000 N, or 108 kN. Divide by 9.81 for tonnes: 9.8 and 11.0.
Mass is not in the clamp formula; area is. A 110 g part can need more clamp than a heavier one if it spreads wider on the parting line. Box one part at 38×38 mm and the envelope is 1,444 mm², but the cross fills only part of that box: 110 g of Zamak at 24 mm thick is about 700–800 mm² of actual projected area, 21–24 kN at 30 MPa. The cross leaves four corners open, so the metal footprint is smaller. Four boxes would overstate the tool. On the layout, four cavities plus runner total 3,200–3,600 mm², which is 96–108 kN at 30 MPa. Against 245 kN, the layout uses 39–44% of the clamp. At 35 MPa the demand is 112–126 kN, about 11 tonnes.
Projected area grows with the square of the outline. Take the same cross to 76×76 mm: the box goes from 1,444 to 5,776 mm², four times the area. One cavity at 30 MPa then asks for 173 kN. Four cavities of the larger cross would need about 693 kN, nearly three times the rating; the 110 g part stays inside it. A clamp shortfall shows as flash at the parting line, and the die halves flex apart; the parting edges wear faster. Shot size has its own ceiling: four parts at 110 g plus runner and overflow must fit the shot end. A heavier part can run out of shot before it runs out of clamp. No nameplate states a maximum part weight.
Send the drawing with the 38×38 mm outline, the 110 g mass, Zamak 5 to ASTM B86 AC41A, and the cavity count. State the machine and the pressure window, 25–35 MPa. Ask for two numbers per part: projected area and shot weight with its share of the runner. Ask what clamp the layout needs at 30 MPa, and what the machine's area ceiling is at that pressure. Do not ask for a maximum part weight. That answer moves with pressure, cavity count, and runner; a gram figure is not a machine rating. Give the limit per part so a 1×4 tool and a single-cavity tool compare.
| Item | Figure | Check |
|---|---|---|
| Part envelope, 38×38 mm | 1,444 mm² | Box the outline; corners open |
| Projected area, one part | 700–800 mm² | 110 g at 24 mm; CAD check |
| Four cavities plus runner | 3,200–3,600 mm² | CAD area of the layout |
| Clamp demand at 30 MPa | 96–108 kN (9.8–11 t) | Area × 30 N/mm² ÷ 9.81 |
| Machine rating | 245 kN (25 t) | Required / rating = 39–44% |
| Pressure window | 25–35 MPa, typical | Plunger setting; 35 MPa gives 112–126 kN |
| Shot weight | 110 g per part, plus runner | Capacity stated per part |
Before fixing the layout, send the drawing for a manufacturability review with the outline, cavity count, and pressure window marked.