A clamp block does not need the strongest zinc alloy. It needs one that holds an M10 screw at 16 mm engagement without the thread or slit walls creeping under sustained preload. This 110±10 g cross clamp block therefore specifies Zamak 5 (ASTM B86 AC41A), not Zamak 3. The difference is about 1% copper, and it matters most in the thread.
The part is a 38×38×24 mm zinc die casting: 18.0±0.1 mm arms, Ø20×4 mm center boss. The M10×1.5 thread runs 16 mm deep; the slit is 1.0±0.1 mm by 22 mm, checked at mid-depth with a 0.10 mm feeler. The bottom face holds 0.05 mm flatness.
Both, in series. The thread turns torque into axial preload. The slit turns that preload into clamping movement. A stripped thread or a bottomed slit leaves the joint loose, but in different places.
The thread is 16 mm deep in a 24 mm block, so engagement spans two-thirds of the body. The first threads take most of the load; the root concentrates stress. The 22 mm slit leaves a hinge at its end. The 0.10 mm feeler at mid-depth must stop: a slit that still takes the blade there has stayed open, and the clamp faces cannot seat.
The alloy sees shear in the thread and bending at the slit root for months. Creep decides more than one-time tensile strength.
Both are zinc-aluminum hot-chamber alloys at about 4% aluminum. Zamak 3 has no intentional copper. Zamak 5 adds about 1% copper, gaining tensile strength and creep resistance while losing some elongation. Zamak 3 is more ductile and easier to plate; Zamak 5 is stronger under sustained load. At room temperature the tensile difference is real; the creep difference is larger.
| Alloy | Property | Fit |
|---|---|---|
| Zamak 3 (AC40A) | No intentional copper; highest ductility, best plating and forming; lower creep strength | Formed or decorative parts with light thread load |
| Zamak 5 (AC41A) | About 1% copper; higher tensile and creep resistance; slightly lower ductility | This clamp. M10 thread and slit hold preload |
| Zamak 7 | Lower magnesium; better fluidity; lower strength than Zamak 5 | Thin walls or long flow paths |
| ZA-8 | About 8% aluminum; higher strength and wear resistance | Wear-led joints and bushings; over-spec here |
The thread decides it. M10×1.5, 16 mm deep, in a block, with a screw tightened hard. Copper raises creep resistance, so preload survives. The slit flexes as the screw closes it; that is not a forming operation.
Stiffness is mostly geometry. Zinc alloys have similar modulus, so Zamak 5 does not make the arms stiffer. It keeps clamp load from bleeding away, so the joint still feels tight months later.
Plating does not decide it. The option is a trivalent chrome conversion film under 0.1 µm, not decorative chrome. Zamak 3's plating edge would matter on a visible nickel-chrome part. There is no T6; the alloy is used as cast, and a T6 callout would risk the 0.05 mm flatness.
Zamak 3 wins when ductility is the constraint. A cover or bracket formed or staked after casting suits it, as does a lightly loaded plated part. A clamp held under screw preload does not.
ZA-8 wins when wear or peak load is the constraint: a sliding joint or a bushing surface. Higher aluminum brings a different casting window, so it is not a drop-in for a tool built around Zamak 5.
One line: "Material: Zamak 5, ASTM B86 AC41A. No T6." Add "as cast" if routing needs it. Spell out the grade; "Zamac" is a misspelling and "zinc alloy 5" is not a grade. Ask for a material certificate with the lot number, not a property table on the drawing.
Keep the process window on the tool card: melt 400–420 °C, mold 170–190 °C, injection 25–35 MPa, 1×4. Add the finish only when specified: trivalent chrome passivation, clear, under 0.1 µm.
The features do the work: 110±10 g, 38×38×24 mm, arms 18.0±0.1 mm, boss Ø20×4 mm, thread 16 mm deep, slit 1.0±0.1×22 mm with the 0.10 mm feeler, bottom flatness 0.05 mm. Put the alloy callout in the title block, beside those dimensions.
Before the alloy line is fixed, send the drawing for a manufacturability review. Mark the thread depth, the slit, and the flatness datum; those test the alloy choice.