The die casting thread crack starts at the root because the saw cuts a finished M10×1.5 thread that already carries tensile stress. A 1.0 mm blade opens the ring in one pass, and the root, not the open slit, is the sharpest notch left in the load path. Saw the slit before the tap to avoid it.

A 110±10 g clamp block is a Zamak 5 (ASTM B86 AC41A) zinc die casting with 18.0±0.1 mm arms and a Ø20×4 mm boss. The M10×1.5 thread is 16 mm deep, and a 1.0±0.1 mm slit is 22 mm deep and crosses it. The order matters.

What happens when the saw meets a tapped thread?

The blade cuts 22 mm through the arm and breaks into the 16 mm deep bore. At that point, the cut is interrupted, and one or two teeth carry the whole chip load for part of the pass. The finished thread has no stock to absorb the push, so tooth impact and released casting stress reach the root together.

Opening the cut lets the Ø20 mm boss relax out of round. The movement is small, but the root is a 60° notch with a radius smaller than the 1.0 mm saw cut. The slit opens; the root takes the bending.

Why does the thread root crack instead of the slit?

A crack needs a ligament, an uncut bridge of metal. The slit has none: its two faces are free once the blade passes. The thread root is the nearest continuous notch to the slit that still carries load, so a crack starts there.

Tapping cuts the root notch and cold-works its flanks. With melt at 400–420 °C and mold at 170–190 °C, the Ø20 mm boss freezes last, so the thread ring holds residual stress before the saw arrives. Removing the ring support sends that stress through the remaining thread. A crack follows the root pitch by pitch. The slit widens; it does not crack.

Which process order avoids it?

Cut this slit before the M10 tap. Cast, trim, saw a 1.0 mm slot 22 mm deep, holding ±0.1 mm, tap the 16 mm deep thread, then deburr both cut edges. The saw never touches a finished thread; the tap then cuts the interrupted profile in its final stress state. The go/no-go gage reads the finished thread.

This order adds a deburr step after tapping, because the tap can drag a burr across the slit. That sequence is what keeps the saw off the thread. If the route stays tap-then-saw, a threaded support plug and a fine-tooth blade cut the risk; they do not take the finished thread out of the cut.

How is the thread checked after sawing?

After tapping, clean the slit and gage the thread with an M10×1.5 go/no-go plug gage. The go member must pass the full 16 mm by hand. The no-go member must stop at the thread entry. A gage that needs force is a fail, because forcing it can open the crack.

Look at both cut edges under 10× before gaging. A chipped flank or a dark line along the root is a reject, even if the gage passes. At mid-depth, a 0.10 mm feeler confirms the cut is open; a pin gage reads the 1.0 mm width to ±0.1 mm. Repeat the gage after passivation.

ParameterTarget (mm or condition)Check
M10×1.5 thread16 mm, full threadGo/no-go gage; go by hand, no-go stops
Thread rootNo crack or chip10× at both cut edges
Slit1.0 mm wide, ±0.1 mm; 22 mm deep0.10 mm feeler at mid-depth; pin gage; depth gauge
Bottom face0.05 mm flatnessPlate; 0.05 mm blade must not enter

What should the drawing specify?

The drawing should sequence the saw before the tap: slit 1.0±0.1 mm wide and 22 mm deep, then M10×1.5, 16 mm deep, full thread by go/no-go. Put the slit callout on the view showing its intersection with the bore. Add the edge deburr and the 10× root check to the notes.

Call out Zamak 5 to ASTM B86 AC41A, as cast, no T6. Show the 38×38×24 mm outline, 18.0±0.1 mm arm width, Ø20×4 mm boss and 110±10 g mass. Hold the bottom face to 0.05 mm flatness. Call out trivalent chromium passivation below 0.1 µm; it does not change the thread or slit.

The crack follows the process order. To check that order, send the drawing for a manufacturability review with the thread and slit callouts marked before the first cut.