A 1.0 mm saw cut after tapping chipped the M10 thread in a Zamak 5 clamp block, and no plug gage felt it. The first route tapped the bore, then sawed into it: the blade broke through the finished flanks, released stress closed the kerf on the blade, and the edge chipped. Sawing first removed the chip. The part is a 110±10 g zinc die casting, 38×38×24 mm, from a 1×4 H13 tool.
Four arms at 18.0±0.1 mm sit around a Ø20×4 mm boss. An M10×1.5 thread runs 16 mm deep from the top face; a 1.0±0.1 mm slit, 22 mm deep, cuts into the bore from the same face, so the boss becomes a C hinged on a 2 mm web.
A clamp screw turns torque into preload, and the slit lets the boss flex so the block closes on a bar. Zamak 5 to ASTM B86 AC41A carries the thread load because about 1% copper raises creep resistance under sustained load, which the pull-out tests for Zamak 5 threads check.
The first route ran cast, trim, tumble deburr, tap, then saw. Tapping a closed ring is the easy case: the teeth are supported all round.
A 1.0 mm blade enters beside the bore and cuts 22 mm down. Partway down it breaks into the threaded bore, so one side runs in air while the other rubs finished flanks, and the kerf closes behind it as the casting relaxes.
Tapping made it worse: it notches and cold-works the flanks while the boss holds stress from uneven freezing, and opening the ring lets the bore shift out of round by micrometres during the cut.
A chip hides from a plug gage: bearing area drops, pitch diameter holds, so go passes and the joint fails later. A burr stops go and sends good thread to rework.
The route now reads cast, trim, tumble deburr, saw the slit, tap and bench deburr, clean, gage, optional passivation. The kerf closes before any flank exists, and the thread is cut after the stress moves.
Tapping an interrupted bore is the tradeoff: the thread opens into a C, the tap loses one flank for part of each turn, and the load pulls it toward the open side.
Tumble stays ahead of the saw: it removes casting flash, not cut edges, and its media cannot enter a 1.0 mm slit. That burr goes to the bench deburr, within the limit the thread and slit design guidelines set. The order changes the quote: sawing after tapping prices a different part.
Four settings held:
| Melt (°C) | Die (°C) | Injection (MPa) | Cycle (s) |
|---|---|---|---|
| 400–420 | 170–190 | 25–35 | 25–35 |
The print carries one note beside the thread callout, slit before tap, because a shop reading only that callout taps first.
Tumble runs before the saw and never after; the bench deburr follows each tap. Trivalent chromium passivation stays optional, masked at threads and slit faces with the film below 0.1 µm, as the finishing options for zinc die cast parts describe.
An M10×1.5 go/no-go plug gage checks the thread: go passes the full 16 mm by hand, no-go stops at the entry, and force is a fail.
Width and closure read separately. At the mouth, a 0.9 mm pin must enter and a 1.1 mm pin must not; at 11 mm, a 0.10 mm feeler must not enter. That depth is the reading to keep, because the blade has no side support, the top edge keeps a burr, and a 22 mm cut can wander. Clamped, the slit reads closed for the wrong reason.
| Check | Gage | Criterion (mm) | Depth (mm) |
|---|---|---|---|
| M10×1.5 thread | go/no-go plug | go by hand, no-go stops | 16 |
| Slit at mouth | 0.9 and 1.1 pins | 0.9 in, 1.1 refuses | 0 |
| Slit closure | 0.10 mm feeler | no entry | 11 |
| Bottom face flatness | plate and 0.05 mm feeler | no entry at corners | whole face |
A 10× look at both thread edges precedes the gage, mass is read at 110±10 g on the first piece, and the checks repeat after passivation, which the quality control routine for mass production treats as a release step.
Cut before the thread whenever a secondary cut crosses it. A thread is slow to repair and easy to protect, and the release happens in metal with no thread to damage.
The rule has edges. A clearance slot that never closes needs width at depth, not a feeler; a rolled thread changes the order; heat treatment after tapping gives the saw competition.
The case proves one sequence: slit first, gage last. This case does not prove the 48 h salt spray result to ASTM B117, or that a later lot will gage the same. A Zamak 5 bank body ran the same one-stop route. For this conflict, send the drawing for a manufacturability review with both features on one view.